Back to Blog
    Technical Guide· 8 min read·10 November 2026

    The Cobalt Binder in WC-Co Cemented Carbide: What It Does and How It Interacts with Your WC Powder

    Cemented carbide is tungsten carbide grains held together by a metal binder, and in the overwhelming majority of grades that binder is cobalt. The amount of cobalt, and how it behaves during sintering, sets most of the properties a carbide producer cares about. But the binder never works alone — the WC powder's grain size and carbon content decide whether the cobalt can do its job. This article explains the binder side of the system and what it means for how you specify WC powder.

    Why tungsten carbide needs a binder

    Tungsten carbide on its own is extremely hard but brittle, and it is very difficult to sinter to full density without a liquid phase. Cobalt solves both problems. It wets tungsten carbide exceptionally well, dissolves some tungsten and carbon at sintering temperature to form a liquid that pulls the WC grains together, and then solidifies into a tough metallic network that stops cracks from running straight through the carbide.

    The result is a composite: a hard skeleton of WC grains, typically making up 70–97% of the weight, with cobalt filling the spaces between them.

    Cobalt content vs hardness and toughness

    Cobalt content is the main trade-off dial. More cobalt means thicker binder layers between grains: toughness and transverse rupture strength go up, hardness and wear resistance go down. Less cobalt does the opposite.

    Typical ranges, as a rough guide: around 3–6% cobalt for wear-resistant and fine cutting grades; around 6–12% for general-purpose cutting tools and wear parts; around 10–15% for mining, rock-drilling and road-milling grades that take impact; and higher levels, up to 20–30%, for heavy-impact tools and forming dies.

    Cobalt content does not act alone. WC grain size moves the same two properties: finer grains raise hardness, coarser grains raise toughness. A grade designer chooses the pair together — fine WC with low cobalt for maximum hardness, coarse WC with high cobalt for maximum toughness, and many combinations in between.

    What happens during liquid-phase sintering

    Pressed WC-Co parts are sintered at roughly 1,350–1,500 °C, above the temperature at which the cobalt-rich phase becomes liquid. The liquid wets the WC grains, capillary forces pull them together, and the part shrinks substantially — linear shrinkage of around 17–22% is common — as porosity closes.

    During this stage, small WC grains dissolve into the liquid and reprecipitate on larger ones, so the average grain size grows. Fine and sub-micron grades therefore usually include grain-growth inhibitors, most commonly vanadium carbide and chromium carbide, to hold the fine structure.

    This is also why WC powder grain size distribution matters, not just the average F.S.S.S. value. A powder with a long tail of very fine particles feeds grain growth and can produce abnormally large grains in the sintered part.

    The carbon window

    The single most important interaction between binder and WC powder is carbon balance. WC-Co is only two-phase — WC plus cobalt binder — within a narrow range of total carbon.

    If carbon is too low, a brittle mixed carbide called eta-phase (of the W₃Co₃C or W₆Co₆C type) forms, consuming binder and embrittling the part. If carbon is too high, free graphite precipitates as carbon porosity, again reducing strength.

    The window is narrow enough that carbon picked up from wax or lubricant, or lost to oxygen during sintering, can push a grade out of it. Carbide producers usually adjust carbon at the mixing stage to compensate for their own process. To do that reliably they need to know exactly what carbon the WC powder brings in, lot by lot — which is why total carbon and free carbon belong on every WC certificate of analysis as separate figures.

    Magnetic tests: reading the binder without cutting the part

    Because cobalt is ferromagnetic, two non-destructive magnetic measurements are standard quality checks in carbide production.

    Magnetic saturation reflects how much tungsten and carbon are dissolved in the cobalt binder. It falls as dissolved tungsten rises, which happens on the low-carbon side of the window, so it works as an indirect carbon check and an early warning of eta-phase risk.

    Coercive force (coercivity) relates to how finely the binder is divided between WC grains. Finer WC grains and lower cobalt give higher coercivity, so it is used to monitor grain size and grain growth from lot to lot.

    If these numbers drift while your process has not changed, the WC powder lot is one of the first things to check.

    Alternative binders, and what does not change

    Nickel and nickel-chromium binders are used where corrosion resistance or non-magnetic properties are needed, for example in some valve, pump and seal components. Iron-nickel-cobalt binder systems have also been developed, partly because cobalt supply is geographically concentrated and cobalt metal powder is subject to increasingly strict hazard classification and workplace exposure limits in several jurisdictions.

    Whatever the binder, the WC side of the system stays the same: grain size, grain size distribution, total carbon, free carbon, oxygen and impurities. Jayanth Tungsten supplies WC powder in F.S.S.S. grades from fine to coarse with total and free carbon stated per lot; the binder and its addition remain under the carbide producer's control.

    Need tungsten powder for your application?

    ISO 9001:2015 certified · Certificate of analysis with every shipment · WhatsApp replies within a few hours

    WhatsApp Enquiry

    Frequently asked questions

    Why is cobalt used as the binder in tungsten carbide?

    Cobalt wets tungsten carbide exceptionally well, forms a liquid phase that lets WC sinter to full density at around 1,350–1,500 °C, and solidifies into a tough metallic network that resists crack growth. No other common binder matches that combination, which is why WC-Co dominates cemented carbide.

    How does cobalt content affect tungsten carbide properties?

    More cobalt increases toughness and transverse rupture strength but lowers hardness and wear resistance. Less cobalt does the opposite. Wear-resistant grades often use about 3–6% Co, general-purpose grades 6–12%, mining grades 10–15%, and heavy-impact grades up to 20–30%.

    What is eta-phase in cemented carbide?

    Eta-phase is a brittle mixed tungsten-cobalt carbide (W₃Co₃C or W₆Co₆C type) that forms when the carbon content of WC-Co is too low. It consumes binder and weakens the part. Avoiding it requires knowing the WC powder's total carbon precisely and adjusting the mix accordingly.

    Does Jayanth Tungsten supply cobalt powder?

    No. We manufacture tungsten carbide powder, tungsten metal powder, fused tungsten carbide and tungsten chemicals. Carbide producers add their own binder; we supply WC powder with F.S.S.S. grain size, total carbon and free carbon stated on the certificate of analysis for each lot.